SlideShare a Scribd company logo
International Research Journal of Engineering and Technology (IRJET) e-ISSN: 2395-0056
Volume: 06 Issue: 10 | Oct 2019 www.irjet.net p-ISSN: 2395-0072
© 2019, IRJET | Impact Factor value: 7.34 | ISO 9001:2008 Certified Journal | Page 499
Behaviour of RC Slabs with Recycled Aggregates Subjected to Static and
Impact Loading
Chandraiah T S1, Kiran T2
1M.E Student, UVCE, Bangalore, Karnataka, India
2Associate Professor UVCE, Bangalore, Karnataka, India
-------------------------------------------------------------------------***------------------------------------------------------------------------
Abstract: The waste, generated in the construction, maintenance, repair and disposal phases of a building, is called
Construction and Demolition (C&D) Waste. Management of C&D waste is a problem faced not only in India but by the global
community and quantum of waste produced occupies a huge fraction of the total solid waste generation by mass. This
research work aims at making one such experiment where recycled aggregates are produced from C&D waste thus paves a
way, for the effective management of concrete debris. The concrete waste was collected from the waste yard in the college
campus, segregated, crushed in jaw crusher, sieved, washed and used for concreting for a mix proportion of M25, as a
replacement for natural coarse aggregates in proportions of 0%, 30%, 60% and 100%. On testing, the compressive strength
was found to be increasing and split tensile strength and flexural strength were observed to be nearly equal to that of normal
concrete mix. Therefore, use of recycled concrete aggregate showed acceptable performance with respect to mechanical
properties. The recycled aggregates obtained from waste concrete are more angular and have higher absorption and specific
gravity than natural coarse aggregates and it resulted in increased strength and improved load carrying capacity. However,
further studies to determine the effect on durability and improvement on workability are necessary.
Keywords: Recycled aggregates, Natural aggregates, Impact test, Static test, First crack and Ultimate failure.
1. INTRODUCTION
Concrete is the premier construction material across the world and the most widely used in all types of civil engineering
works. Among the ingredients for concrete, aggregates, i.e. inert granular materials such as sand, crushed stone or gravel
form the major part. This is mainly because of the running down of quality primary aggregates and greater awareness of
environmental protection. Hence the use of recycled aggregate from construction and demolition waste (C&D waste) in
concrete is gaining momentum these days. Recycled aggregate concrete may become the need of the day in the years to
come. Crushed stone or gravel form the major part. In recent years due to continued large scale extraction, use of
aggregates from natural resources has been questioned at international level.
1.1 Literature Review
T. Naresh Kumar1, N.Venkata Ramana2, E. Arunakanthi3 and C. Sashidhar4 This paper presents the
Behaviour of stone waste aggregate (SWA) concrete slabs under impact loading. The stone waste was obtained during
extraction of layered stone (at mines) and at polishing stone industries. This stone waste is converted in useful aggregate
and used in the concrete as coarse aggregate in the place of natural aggregate with replacement levels of 0, 25, 50, 75 and
100%. For each replacement level, three slab specimens were cast and tested. 0% replacement level consider as Natural
Aggregate Concrete (NAC) slabs. The SWA slabs were compared with natural aggregate concrete (NAC) slabs. The results
showed that the SWA slab performance is less than the natural aggregate concrete slabs. From experimental results,
regression models were developed to estimate energy absorption at first and ultimate crack stages. In addition to the slab
specimens cubes were cast and tested. The cube strength results were used during development of regression models.
HardikGandhi1, Dr. DharshanaBhatt2 and Chetnaben Vyas3 studied that There is a critical shortage of virgin aggregates
and hence the availability of demolished concrete for use as recycled concrete aggregate (RCA) is increasing. Using the
waste concrete as RCA conserves virgin aggregates, reduces the impact on landfills, decreases energy consumption and
can provide cost savings. Recycled aggregates are comprised of crushed, graded inorganic particles processed from the
materials that have been used in the constructions and demolition debris. Recycled aggregates for application in high
strength structural concrete, which will give a better understanding on the properties of concrete with recycled aggregate,
as an alternative material to coarse aggregate in structural concrete. In the present study recycled coarse aggregate have
been used to replace virgin coarse aggregate. The properties of fresh as well as hardened concrete made of partial/full
replacement of recycled coarse aggregate are found out and the results are compared with that of concrete using virgin
coarse aggregate.
International Research Journal of Engineering and Technology (IRJET) e-ISSN: 2395-0056
Volume: 06 Issue: 10 | Oct 2019 www.irjet.net p-ISSN: 2395-0072
© 2019, IRJET | Impact Factor value: 7.34 | ISO 9001:2008 Certified Journal | Page 500
2. MATERIALS AND METHODOLOGY
2.1 Cement
Cement paste is the binder in concrete that holds the aggregate (coarse, fine, micro fine) together and reacts to form
hardened mass. The property of concrete depends on the quantities and the quality of its constituents.
In this present investigation Ordinary Portland Cement of 53 Grade with a brand name Ultra Tech (Birla Super) used. Tests
are conducted in accordance with the Indian standards confirming to IS-12269:1987. The physical characteristic of the
tested cement has been shown in table 2.1
Table 2.1: Physical Characteristics of Cement
Physical Properties of Cement
Test Results
Requirements as per IS
12269: 1987
Specific Gravity 3.20 3.15
Fineness of cement 2.83% Less than 10%
Standard Consistency 32% Not Specified
Soundness (Le- chatelier’s) 0.5mm Shall not be more than 10mm
Setting time (in minutes)
Initial Setting time 105 Shall not be less than 30 minutes
Final Setting Time 510 Shall not be more than 600 minutes
Compressive Strength (Mpa) (70.5x70.5x70.5mm )
3 Days Strength 38.7 MPa Shall not be less than 27.0 MPa
7 Days Strength 48.2 MPa Shall not be less than 37.0 MPa
28 Days Strength 56.8 MPa Shall not be less than 53.0 MPa
2.2 Fine Aggregate
HPC contains a large quantity of fine cementations materials. Grading of FA should not cause increase in water demand for
concrete. It is desirable to use a coarser variety of sand having high fineness modulus. Both natural sand and crushed stone
dust can be used as fine aggregate, should consists of rounded particles to reduce water demand. Generally, fractions
passing through 4.75 mm sieves and entirely retained on 150µ sieve are used. Locally obtained manufactured sand was
used as the fine aggregate in the concrete mix.
The test on fine aggregate was conducted in accordance with IS: 650-1966 & IS: 2386-1968 to determine specific gravity
and fineness modulus.
Table: 2.2 Physical Characteristics of Fine Aggregate
Sl. No. Particular of Test Results
1 Fineness Modulus 2.3
2 Specific Gravity 2.608
3
Bulk Density (kg/m3)
Dense rodded
1736
1560
4 Zone II
International Research Journal of Engineering and Technology (IRJET) e-ISSN: 2395-0056
Volume: 06 Issue: 10 | Oct 2019 www.irjet.net p-ISSN: 2395-0072
© 2019, IRJET | Impact Factor value: 7.34 | ISO 9001:2008 Certified Journal | Page 501
2.3 Coarse Aggregate
Coarse aggregates passing 12.5 mm sieve size and retained on 10 mm sieve were used. The sieve analysis of combined
aggregates confirms to the specifications of IS 383: 1970 for well graded aggregates. The tests on the coarse aggregate
were conducted in accordance with IS 2386-1963 to determine Specific gravity, Bulk density and Fineness modulus. The
results were presented in Table 2.3
Table 2.3: Physical Properties of Coarse Aggregates (12.5mm down size)
Sl. No. Particulars Results As Per Is:383-1970
1 Fineness Modulus 4.2 ---
2 Specific Gravity 2.63 ---
3 Bulk Density (Dry-Rodded) 1673 Kg/m3 ---
4 Elongation Index 11% 15%
5 Flakiness 13.8% 15%
Crushing Value 24.8% 30% (Max)
7 Impact 17.8% 30% (Max)
8 Los Angeles Abrasion value 29.9% 30% (Max)
2.3 Recycled aggregate concrete (RAC)
There are many reasons why concrete has been the most widely used material in the world for many decades now. The
most advantageous characteristics of concrete can be listed as: relatively low cost, grand scale availability of its raw
components, durability, workability, how adaptable concrete is to be shaped into any form and its fire resistance. But there
is a price to pay for all these benefits, namely, the colossal energy consumption and devastating pollution that results from
the manufacturing of cement.
To reduce this impact and achieve a more sustainable product, waste materials can be incorporated into concrete in the
form of RA. The most extensively researched material used in the production of RA is waste concrete, that is, fine and
coarse debris from demolition sites. Also, less common components such as glass, coal fly ash, plastic, tyres, volcanic ash
and foundry sand have been investigated by several researchers. Concrete with RA as a component in the mixing process
is referred to as recycled aggregate concrete. Since aggregates are a vital part of concrete, and concrete is widely used in
the world today, this thesis presents a brief literature review on the use of RA in the production of concrete, the end
product is referred to as recycled aggregate concrete (RAC). The aim of this review is to establish the mechanical
properties of RAC and to compare results with the mechanical performance of conventional concrete, that is, concrete
made of aggregates that did not incorporate recycled materials as aggregate.
3. LABORATORY INVESTIGATIONS
3.1 Design of Slabs
Table: 3.1The details of the slab design
Thickness
(mm)
Dimension of slab
(mm)
Main
Distribution
Length
(mm) spacing
Mai
n
Distribution
50 600X600 6 6 550 550 80 mm c/c
International Research Journal of Engineering and Technology (IRJET) e-ISSN: 2395-0056
Volume: 06 Issue: 10 | Oct 2019 www.irjet.net p-ISSN: 2395-0072
© 2019, IRJET | Impact Factor value: 7.34 | ISO 9001:2008 Certified Journal | Page 502
3.2 Casting of Slab Specimens
This part deals with the casting of reinforced slab specimens. Totally eighteen reinforced concrete slabs were cast and
tested, the sizes of the test specimens were selected to suit the capacity of test equipment available in the laboratory. The
slabs are designed as two-way slabs by treating as an interior panel (all four sides continuous). The live load considered
for this study is 8 kN/m2 and the design is as per IS- 456:2000. The design details of all twelve slabs are as given below in
the table. The design of slabs in detail are shown in above table 3.1.
All slabs were (600 X 600) mm with thickness of 50 mm. All the slabs were designed as two-way slabs. The tensile
reinforcement ratio varied according to the thickness of slabs. The clear cover to reinforcement was 15 mm on all faces.
The typical details of the pattern of the reinforcement and cross section of the slabs are shown in Fig 3.6. Totally twelve
(six for static test and six for impact test) test slab specimens are named sequentially as CS, CS + 10%, CS + 20%, CS + 30%,
CS+40%, CS+50% were casted. After 24 hours, test specimens were demolded and the test specimens were cured
continuously for 28 days. Details of Slabs are given below.
Totally twelve (six for static test and six for impact test) test slab specimens are named sequentially as CS, CS + 10%, CS +
20%, CS + 30%, CS+40%, CS+50% were casted. After 24 hours, test specimens were demolded and the test specimens
were cured continuously for 28 days. Details of Slabs are given below
Slno Slabs No of Specimens
1 M30 2
2 M30+10%RCA 2
3 M30+20%RCA 2
4 M30+30%RCA 2
5 M30+40%RCA 2
6 M30+50%RCA 2
3.3 Casting of Cubes and Prisms
3.3.1 Casting of cubes (150*150*150mm) and prisms (100*100*500mm)
 Initially moulds are cleaned and oiled. The next step involved fixing the mould end plates using nuts and bolts.
 Weigh the amount of cement, silica fume, GGBS, fine aggregates and coarse aggregates for moulds. Materials were
first dry mixed, then mixed with 1/3rd amount of total water with super plasticizer and polypropylene and steel
fibre are added to M30 concrete. Remaining water was then added and mixed thoroughly to get homogeneous mix.
 Then the mould was fully compacted by using the vibrating machine. Sufficient care was taken to see that concrete
was properly filled in corners and the edges of the mould. As soon as the air bubbles stopped to rise, the top surface
of the mould was finished with trowel by applying little pressure.
3.3.2 Curing
After 24 hrs concrete specimen are removed from the moulds and kept for curing in water bath for the required days of
curing. All Specimens are cured for 3 days, 7 days & 28 days as per standard procedure.
International Research Journal of Engineering and Technology (IRJET) e-ISSN: 2395-0056
Volume: 06 Issue: 10 | Oct 2019 www.irjet.net p-ISSN: 2395-0072
© 2019, IRJET | Impact Factor value: 7.34 | ISO 9001:2008 Certified Journal | Page 503
4. MECHANICAL PROPERTIES
Testing of hardened concrete place an important role in controlling and confirming the quality of cement concrete works.
Systematic testing of raw materials, fresh concrete and hardened concrete are inseparable part of any quality control
program for concrete which helps to achieve higher efficiency of the material used and greater assurance of the
performance of concrete with regard to both strength and durability. One of the purposes of testing hardened concrete is
to confirm that the concrete used at site has developed the require strength. As the hardening of concrete takes time one
will not come to know the actual strength of concrete for some time. Tests are made by casting cubes or cylinders from the
representative concrete or cores cut from the actual concrete.
4.1 Compressive strength
The compressive strength of concrete i.e. ultimate strength of concrete is defined as the load which causes failure of the
specimen divided by the area of the cross section in unit- axial compression, under a given rate of loading i.e., 13.73
N/mm2. To avoid large variation in the results of compression test, care should be taken during the casting of the test
specimens and loading as well.
The cube mould of 150mm x 150mm x 150mm size is taken as per IS: 516-1959 specification. The cubes were tested in
200T capacity compressive testing machine. Place the specimen in the machine then apply the load continuously,
uniformly and without shock. The rate of loading is continuously adjusted in Newton’s through rate control valve by hand.
The load is increased until the specimen fails and record the maximum load carried by specimen during the test. Fig 1
shows the testing of cube specimen in progress. The compression strength is calculated using the formula,
f = P/A
Where, f = is compressive strength of concrete in N/mm2
P = ultimate load resisted by concrete
Fig.1. Compressive testing of Cubes
4.2 Flexural strength
Flexural strength is expressed in terms of “Modulus rupture” which is the maximum tensile (or compressive) stress at
rupture.
Modulus of rupture
Modulus of rupture is defined as the normal tensile stress in concrete, when cracking occurs in a flexure test. This tensile
stress is the flexural strength of concrete and is calculated by the use of the formula, which assumes that the section is
homogeneous.
fb = (p x l) / (b x d2)
Where,
International Research Journal of Engineering and Technology (IRJET) e-ISSN: 2395-0056
Volume: 06 Issue: 10 | Oct 2019 www.irjet.net p-ISSN: 2395-0072
© 2019, IRJET | Impact Factor value: 7.34 | ISO 9001:2008 Certified Journal | Page 504
fb = modulus of rupture, N/mm2
b = measured width in mm of the specimen
d = measured depth in mm of the specimen at the point of failure
l = length in mm of the span on which specimen was supported
p = max. Load in N applied to the specimen
 Prisms are tested immediately on removal from the water while they are still in wet condition. The bearing surfaces
of the supporting and loading rollers are wiped clean, and loose sand or other material removed from the surfaces
of specimen where they are to make contact with the rollers. The specimen is then placed in the machine in such a
manner that the load is applied to the uppermost surface as cast in the mould, along two lines spaced 13.3cm apart
(If the fracture occurs within the middle third of the span, a>133mm, fb = pl/bd2.
 If the fracture occurs outside the middle third but deviating by not more than 5 percent of the span length,
110<a<133mm
Then, fb = 3PL/bd ²
Where,
P= Load
L = span in mm
a= distance between line of fracture and the nearest support in mm
b = average breadth of the specimen in mm
d = average depth of the specimen in mm
If fracture occurs by more than 5 percent outside the middle third, a<110mm, then the results of the test should be
rejected.
Fig. 2. Flexural Test on Beam Prisms
5. STATIC TESTING OF SLABS
5.1 General
 A static test setup is fabricated for the test programme, which should have relatively stiff supports and the
hydraulic loading assembly is fixed to the supporting frame. Since the study is mainly aimed at evaluation of static
International Research Journal of Engineering and Technology (IRJET) e-ISSN: 2395-0056
Volume: 06 Issue: 10 | Oct 2019 www.irjet.net p-ISSN: 2395-0072
© 2019, IRJET | Impact Factor value: 7.34 | ISO 9001:2008 Certified Journal | Page 505
response due to load, as also the cumulative effect of such loading on the concrete slab elements, a hydraulic jack
type loading has been employed for Static Testing Machine.
 The static testing machine used in the present investigation is of hydraulic loading type instrumented assembly.
The detailed view of the above machine is shown in Fig. 3.
Fig. 3. Static Test Setup
5.2 Instrumentation
The following instrumentation is used in the present experimental investigation to study the behaviour of the slabs under
static loading. This consists of two Linear Variable Differential Transducers (LVDT), one at center and another at quarter
span and are used to receive displacement variation with time. Load cell attached to the head of the hydraulic jack to
record load time history.
From the literature review it has been observed that a single assembly of instrumentation was not possible. The
incorporation of electronic devices to record the specimen response to different energy level of impact is proved to be very
efficient hence the data acquisition system along with LVDT, accelerometer and load cell is essential. In the present
investigation the dynamic response and other parameters are studied with the help of very sensitive electronic devices.
The response send by these devices are analyzed through a software programme to get actual experimental values. In
addition, the data Acquisition system are used in the present investigation.
5.3 LVDT
LVDT (Linear Variable Different Transformer) is a sensitive device, shown in fig 4. used for measuring minute mechanical
displacements. It consists of LVDT coil Prising of primary and two secondaries wound on an acrylic bobbin. A
ferromagnetic core moves inside the coil. The output is proportional to the displacement. The electric inputs/outputs are
termed on to a 6 – pin MS connector.
Fig. 4. LVDT and its Fixtures
International Research Journal of Engineering and Technology (IRJET) e-ISSN: 2395-0056
Volume: 06 Issue: 10 | Oct 2019 www.irjet.net p-ISSN: 2395-0072
© 2019, IRJET | Impact Factor value: 7.34 | ISO 9001:2008 Certified Journal | Page 506
5. IMPACT TESTING OF SLABS
5.1 General
Since the study is mainly aimed at evaluation of dynamic response due to load, as also the cumulative effect of such blows
on the concrete slab elements, impact test a low velocity drop weight has been employed in the present experimental
investigation.
The main objective of this investigation is to study the load-time variation, displacement-time variation and energy
absorption capacity of slabs under low velocity repeated impact loading. Such data obtained from tests are to be analyzed
to study the behaviour of slab under low velocity repeated impact loading.
5.2 Impact Testing Machine
The impact testing machine used in the present investigation is of low velocity drop weight type instrumented impact
testing machine: The detailed view above machine is shown in Fig 5. The impact testing machine consists of major three
parts are as follows.
In impact test the impact load was applied by means of the free fall of a drop weight from 1m height. For free fall the drop
weight was arranged, to fall between the guided cylinder and impact the specimen at midpoint. The drop weight had a
steel circular load cell of diameter 5.5cm as shown in the fig below.
Fig.5. Impact Test Setup
5.3 Instrumentation
The following instrumentation is used in the present experimental investigation to study the impact behaviour of the slabs
under low velocity drop weight impact loading. This consists of,
 Two Linear Variable Differential Transducers (LVDT), one at center and another et quarter span and are used to
receive displacement variation with time
 An accelerometer are used for recording acceleration time history.
 Load cell attached to the head of striker to record load time history
Fig. 6. Drop Hammer
International Research Journal of Engineering and Technology (IRJET) e-ISSN: 2395-0056
Volume: 06 Issue: 10 | Oct 2019 www.irjet.net p-ISSN: 2395-0072
© 2019, IRJET | Impact Factor value: 7.34 | ISO 9001:2008 Certified Journal | Page 507
From the literature review it has been observed that a single assembly of instrumentation was not possible. The
incorporation of electronic devices to record the specimen response to different energy level of impact is proved to be very
efficient hence the data acquisition system along with LVDT, accelerometer and load cell is essential. In the present
investigation the dynamic response and other parameters are studied with the help of very sensitive electronic devices.
The response sends by these devices are analyzed through a software programmed to get actual experimental values. In
addition, the data Acquisition system are used in the present investigation.
6. TEST RESULTS AND DISCUSSION OF EXPERIMENTAL PROGRAMME
6.1 Compression Test on Standard Cubes
The test is conducted as per IS: 516-1959 (Reaffirmed 2008). The experimental compressive strength values obtained on
standard cube specimen of size 150 mm x 150 mm x 150 mm, cured for 7 days and 28 days for all four different concrete
matrices are presented in the form of graphs and bar charts shown in figure.
Compressive Strength
DAYS M30 M30+10%RCA M30+20%RCA M30+30%RCA M30+40%RCA M30+50%RCA
7 26.37 22.55 24.33 21.77 20.11 18.85
28 34.66 26.03 28.43 24.66 22.88 21.55
International Research Journal of Engineering and Technology (IRJET) e-ISSN: 2395-0056
Volume: 06 Issue: 10 | Oct 2019 www.irjet.net p-ISSN: 2395-0072
© 2019, IRJET | Impact Factor value: 7.34 | ISO 9001:2008 Certified Journal | Page 508
6.2 Static Test Results for Slabs
Combined graph of all Specimens
0
5
10
15
20
25
0 2 4 6 8
Load(Kn)
Deflection (mm)
Load v/s Deflection
M30+30%RCA
0
2
4
6
8
10
12
14
16
18
0 2 4 6 8
Load(Kn)
Deflection (mm)
Load v/s Deflection
M30+50%RCA
International Research Journal of Engineering and Technology (IRJET) e-ISSN: 2395-0056
Volume: 06 Issue: 10 | Oct 2019 www.irjet.net p-ISSN: 2395-0072
© 2019, IRJET | Impact Factor value: 7.34 | ISO 9001:2008 Certified Journal | Page 509
6.3 Impact Test Results for Slab
7. CONCLUSION
In this study it is found that there is not much variation in strength between ordinary concrete and 20% replaced
aggregate concrete, which proves the previous works. But when the percentage of aggregate replaced increases there is a
constant increase in strengths, which is a controversy to the previous works. Because it has been found that recycled
aggregates obtained from recycling concrete are more angular and have higher absorption and specific gravity than
natural coarse aggregates it may result on increase of strength and improved load carrying capacity. However, further
studies to determine the effect on durability and improvement on workability are necessary.
REFERENCES
[1] Tomas U. Ganiron Jr, (2015), “Recycling Concrete Debris from Construction and Demolition Waste”, International
Journal of Advanced Science and Technology Vol.77, pp.7-24.
[2] Roz-Ud-Din Nassar and Previz Soroushian, (2012), “Strength and durability of recycled aggregate concrete containing
milled glass as partial replacement for cement”, Construction and Building Materials, Vol. 29. pp. 368–377
[3] Markandeya Raju Ponnada1 and Kameswari P, (2015), “Construction and Demolition Waste Management – A Review”,
International Journal of Advanced Science and Technology, Vol. 84, pp.19-46.
[4] Jitender Sharma and Sandeep Singla, (2014), “Study of Recycled Concrete Aggregates” `, International Journal of
Engineering Trends and Technology (IJETT), Vol. 13, No. 3, pp. 123 – 125.
0
1
2
3
4
0
1
2
3
4
5
0 5 10 15
Displacementmm
NO OF Blows
ALL SPECIMENS
M30+1
0%RCA
M30+2
0%RCA
M30+3
0%RCA
M30+4
0%RCA

More Related Content

PDF
IRJET- Partial and Complete Replacement of Sand in Concrete with Waste Glass,...
PDF
20320130406019 2
PDF
IRJET- Manufacturing of Stabilized Blocks using Shedi Soil
PDF
Experimental Investigation on Self Compacting Concrete by Introducing Fly Ash...
PDF
Experimental Study of Mechanical Properties of Concrete using Recycled Aggre...
PDF
IRJET- Mechanical Properties of Fibre Reinforced Concrete using Preserved...
PDF
A Brief Study on the Strength Properties of Concrete Modified With Sintered F...
PDF
IRJET- Strength and Durability Studies on Concrete Made using Treated Recycle...
IRJET- Partial and Complete Replacement of Sand in Concrete with Waste Glass,...
20320130406019 2
IRJET- Manufacturing of Stabilized Blocks using Shedi Soil
Experimental Investigation on Self Compacting Concrete by Introducing Fly Ash...
Experimental Study of Mechanical Properties of Concrete using Recycled Aggre...
IRJET- Mechanical Properties of Fibre Reinforced Concrete using Preserved...
A Brief Study on the Strength Properties of Concrete Modified With Sintered F...
IRJET- Strength and Durability Studies on Concrete Made using Treated Recycle...

What's hot (19)

PDF
IRJET- A Review on Behaviour of ECO Green Concrete in Construction Industry
PDF
IRJET- Reusability of Construction and Demolition Waste in Bricks
PDF
IRJET - Study on High Strength Concrete by using Replacement of Metakaolin an...
PDF
IRJET- Experimental Investigation on Effect of Sand Content in Pervious Concrete
PDF
IRJET- Replacement of Fine Aggregate in Concrete using Construction Demolishe...
PDF
Experimental Study on Performance of Concrete M30 with Partial Replacement of...
PDF
IRJET- Effect of Manufacturing Sand on Durability of Concrete
PPTX
Coconut shell as coarse aggregate in the concrete
PDF
IRJET- Experimental Investigation on Bubble Deck Slab Confining High Density ...
PDF
Investigation on Crushed Materials as Aggregate in Concrete
PDF
PARTIAL REPLACEMENT OF AGGREGATES BY BURNT BRICK BATS AND LATERITIC FINES IN ...
PDF
An Experimental Investigation on Self Compacting Concrete with Artificial Fin...
PDF
A REVIEW PAPER ON PROPERTIES OF CONCRETE WITH FRACTIONAL REPLACEMENT OF RECYC...
PDF
IRJET- A Study on Influence of Graphene Oxide Powder on Compressive Strength ...
PDF
Compressive Strength of Concrete made from Natural Fine Aggregate Sources in ...
PDF
IRJET- Experimental Study on Strength Characteristics of Glass Fibre Reinforc...
PDF
IRJET - Investigation Study on Fine Aggregate Fragmentary Replacement by ...
PDF
Influence of RGO and Fly-Ash on Cement Composite at Elevated Temperatures
PDF
IRJET - Study on Partial Replacement of Cement by Ground Granulated Blast Fur...
IRJET- A Review on Behaviour of ECO Green Concrete in Construction Industry
IRJET- Reusability of Construction and Demolition Waste in Bricks
IRJET - Study on High Strength Concrete by using Replacement of Metakaolin an...
IRJET- Experimental Investigation on Effect of Sand Content in Pervious Concrete
IRJET- Replacement of Fine Aggregate in Concrete using Construction Demolishe...
Experimental Study on Performance of Concrete M30 with Partial Replacement of...
IRJET- Effect of Manufacturing Sand on Durability of Concrete
Coconut shell as coarse aggregate in the concrete
IRJET- Experimental Investigation on Bubble Deck Slab Confining High Density ...
Investigation on Crushed Materials as Aggregate in Concrete
PARTIAL REPLACEMENT OF AGGREGATES BY BURNT BRICK BATS AND LATERITIC FINES IN ...
An Experimental Investigation on Self Compacting Concrete with Artificial Fin...
A REVIEW PAPER ON PROPERTIES OF CONCRETE WITH FRACTIONAL REPLACEMENT OF RECYC...
IRJET- A Study on Influence of Graphene Oxide Powder on Compressive Strength ...
Compressive Strength of Concrete made from Natural Fine Aggregate Sources in ...
IRJET- Experimental Study on Strength Characteristics of Glass Fibre Reinforc...
IRJET - Investigation Study on Fine Aggregate Fragmentary Replacement by ...
Influence of RGO and Fly-Ash on Cement Composite at Elevated Temperatures
IRJET - Study on Partial Replacement of Cement by Ground Granulated Blast Fur...
Ad

Similar to IRJET- Behaviour of RC Slabs with Recycled Aggregates Subjected to Static and Impact Loading (20)

PDF
20320130406018 2
PDF
IRJET- To Study the Effect of Recycled Aggregate in High Strength Concrete
PDF
IRJET- A Study on use of Recycled Aggregate in Standard Mix Design and its Su...
PDF
IRJET- Establishment of Frame of Reference for Management and Reuse of Demoli...
PDF
An Experimental Investigation on Strength Behavior of Concrete by Replacing N...
PDF
Experimental Investigations on Building Demolition Waste Using as a Fine Aggr...
PDF
IRJET- Experimental Investigation on Recycled Aggregates in Concrete
PDF
Use of Demorlished Concrete in Pavement
PDF
Experimental Investigation on Performance of Recycled Concrete Aggregate as C...
PDF
IRJET- Manufacture of Concrete using Solid Waste from Construction Industry
PDF
IRJET- Study on Concrete Replaced with Crushed Concrete Fine Aggregate
PDF
IRJET- Experimental Investigation on Durability Properties of Recycled Aggreg...
PDF
I25038042
PDF
I25038042
PDF
I25038042
PDF
Er.Mihir Shah ReSEARCH PAPER
PPTX
DOC-20231228-WA0004124758967poyhffrt.pptx
PDF
IRJET- Utilization of Recycled Concrete Aggregate for New Construction
PDF
IRJET - Experimental and Analytical Study on High Strength Concrete (M70)...
20320130406018 2
IRJET- To Study the Effect of Recycled Aggregate in High Strength Concrete
IRJET- A Study on use of Recycled Aggregate in Standard Mix Design and its Su...
IRJET- Establishment of Frame of Reference for Management and Reuse of Demoli...
An Experimental Investigation on Strength Behavior of Concrete by Replacing N...
Experimental Investigations on Building Demolition Waste Using as a Fine Aggr...
IRJET- Experimental Investigation on Recycled Aggregates in Concrete
Use of Demorlished Concrete in Pavement
Experimental Investigation on Performance of Recycled Concrete Aggregate as C...
IRJET- Manufacture of Concrete using Solid Waste from Construction Industry
IRJET- Study on Concrete Replaced with Crushed Concrete Fine Aggregate
IRJET- Experimental Investigation on Durability Properties of Recycled Aggreg...
I25038042
I25038042
I25038042
Er.Mihir Shah ReSEARCH PAPER
DOC-20231228-WA0004124758967poyhffrt.pptx
IRJET- Utilization of Recycled Concrete Aggregate for New Construction
IRJET - Experimental and Analytical Study on High Strength Concrete (M70)...
Ad

More from IRJET Journal (20)

PDF
Enhanced heart disease prediction using SKNDGR ensemble Machine Learning Model
PDF
Utilizing Biomedical Waste for Sustainable Brick Manufacturing: A Novel Appro...
PDF
Kiona – A Smart Society Automation Project
PDF
DESIGN AND DEVELOPMENT OF BATTERY THERMAL MANAGEMENT SYSTEM USING PHASE CHANG...
PDF
Invest in Innovation: Empowering Ideas through Blockchain Based Crowdfunding
PDF
SPACE WATCH YOUR REAL-TIME SPACE INFORMATION HUB
PDF
A Review on Influence of Fluid Viscous Damper on The Behaviour of Multi-store...
PDF
Wireless Arduino Control via Mobile: Eliminating the Need for a Dedicated Wir...
PDF
Explainable AI(XAI) using LIME and Disease Detection in Mango Leaf by Transfe...
PDF
BRAIN TUMOUR DETECTION AND CLASSIFICATION
PDF
The Project Manager as an ambassador of the contract. The case of NEC4 ECC co...
PDF
"Enhanced Heat Transfer Performance in Shell and Tube Heat Exchangers: A CFD ...
PDF
Advancements in CFD Analysis of Shell and Tube Heat Exchangers with Nanofluid...
PDF
Breast Cancer Detection using Computer Vision
PDF
Auto-Charging E-Vehicle with its battery Management.
PDF
Analysis of high energy charge particle in the Heliosphere
PDF
A Novel System for Recommending Agricultural Crops Using Machine Learning App...
PDF
Auto-Charging E-Vehicle with its battery Management.
PDF
Analysis of high energy charge particle in the Heliosphere
PDF
Wireless Arduino Control via Mobile: Eliminating the Need for a Dedicated Wir...
Enhanced heart disease prediction using SKNDGR ensemble Machine Learning Model
Utilizing Biomedical Waste for Sustainable Brick Manufacturing: A Novel Appro...
Kiona – A Smart Society Automation Project
DESIGN AND DEVELOPMENT OF BATTERY THERMAL MANAGEMENT SYSTEM USING PHASE CHANG...
Invest in Innovation: Empowering Ideas through Blockchain Based Crowdfunding
SPACE WATCH YOUR REAL-TIME SPACE INFORMATION HUB
A Review on Influence of Fluid Viscous Damper on The Behaviour of Multi-store...
Wireless Arduino Control via Mobile: Eliminating the Need for a Dedicated Wir...
Explainable AI(XAI) using LIME and Disease Detection in Mango Leaf by Transfe...
BRAIN TUMOUR DETECTION AND CLASSIFICATION
The Project Manager as an ambassador of the contract. The case of NEC4 ECC co...
"Enhanced Heat Transfer Performance in Shell and Tube Heat Exchangers: A CFD ...
Advancements in CFD Analysis of Shell and Tube Heat Exchangers with Nanofluid...
Breast Cancer Detection using Computer Vision
Auto-Charging E-Vehicle with its battery Management.
Analysis of high energy charge particle in the Heliosphere
A Novel System for Recommending Agricultural Crops Using Machine Learning App...
Auto-Charging E-Vehicle with its battery Management.
Analysis of high energy charge particle in the Heliosphere
Wireless Arduino Control via Mobile: Eliminating the Need for a Dedicated Wir...

Recently uploaded (20)

PDF
PREDICTION OF DIABETES FROM ELECTRONIC HEALTH RECORDS
PPTX
Fundamentals of safety and accident prevention -final (1).pptx
PDF
Artificial Superintelligence (ASI) Alliance Vision Paper.pdf
PPT
Total quality management ppt for engineering students
PDF
BMEC211 - INTRODUCTION TO MECHATRONICS-1.pdf
PPTX
Construction Project Organization Group 2.pptx
PPTX
CYBER-CRIMES AND SECURITY A guide to understanding
PDF
Mohammad Mahdi Farshadian CV - Prospective PhD Student 2026
PDF
Unit I ESSENTIAL OF DIGITAL MARKETING.pdf
PPTX
Internet of Things (IOT) - A guide to understanding
PDF
III.4.1.2_The_Space_Environment.p pdffdf
PDF
PPT on Performance Review to get promotions
PPTX
Fundamentals of Mechanical Engineering.pptx
PDF
737-MAX_SRG.pdf student reference guides
PPTX
Safety Seminar civil to be ensured for safe working.
PPTX
Foundation to blockchain - A guide to Blockchain Tech
PDF
A SYSTEMATIC REVIEW OF APPLICATIONS IN FRAUD DETECTION
PPTX
MET 305 2019 SCHEME MODULE 2 COMPLETE.pptx
PDF
The CXO Playbook 2025 – Future-Ready Strategies for C-Suite Leaders Cerebrai...
PDF
Human-AI Collaboration: Balancing Agentic AI and Autonomy in Hybrid Systems
PREDICTION OF DIABETES FROM ELECTRONIC HEALTH RECORDS
Fundamentals of safety and accident prevention -final (1).pptx
Artificial Superintelligence (ASI) Alliance Vision Paper.pdf
Total quality management ppt for engineering students
BMEC211 - INTRODUCTION TO MECHATRONICS-1.pdf
Construction Project Organization Group 2.pptx
CYBER-CRIMES AND SECURITY A guide to understanding
Mohammad Mahdi Farshadian CV - Prospective PhD Student 2026
Unit I ESSENTIAL OF DIGITAL MARKETING.pdf
Internet of Things (IOT) - A guide to understanding
III.4.1.2_The_Space_Environment.p pdffdf
PPT on Performance Review to get promotions
Fundamentals of Mechanical Engineering.pptx
737-MAX_SRG.pdf student reference guides
Safety Seminar civil to be ensured for safe working.
Foundation to blockchain - A guide to Blockchain Tech
A SYSTEMATIC REVIEW OF APPLICATIONS IN FRAUD DETECTION
MET 305 2019 SCHEME MODULE 2 COMPLETE.pptx
The CXO Playbook 2025 – Future-Ready Strategies for C-Suite Leaders Cerebrai...
Human-AI Collaboration: Balancing Agentic AI and Autonomy in Hybrid Systems

IRJET- Behaviour of RC Slabs with Recycled Aggregates Subjected to Static and Impact Loading

  • 1. International Research Journal of Engineering and Technology (IRJET) e-ISSN: 2395-0056 Volume: 06 Issue: 10 | Oct 2019 www.irjet.net p-ISSN: 2395-0072 © 2019, IRJET | Impact Factor value: 7.34 | ISO 9001:2008 Certified Journal | Page 499 Behaviour of RC Slabs with Recycled Aggregates Subjected to Static and Impact Loading Chandraiah T S1, Kiran T2 1M.E Student, UVCE, Bangalore, Karnataka, India 2Associate Professor UVCE, Bangalore, Karnataka, India -------------------------------------------------------------------------***------------------------------------------------------------------------ Abstract: The waste, generated in the construction, maintenance, repair and disposal phases of a building, is called Construction and Demolition (C&D) Waste. Management of C&D waste is a problem faced not only in India but by the global community and quantum of waste produced occupies a huge fraction of the total solid waste generation by mass. This research work aims at making one such experiment where recycled aggregates are produced from C&D waste thus paves a way, for the effective management of concrete debris. The concrete waste was collected from the waste yard in the college campus, segregated, crushed in jaw crusher, sieved, washed and used for concreting for a mix proportion of M25, as a replacement for natural coarse aggregates in proportions of 0%, 30%, 60% and 100%. On testing, the compressive strength was found to be increasing and split tensile strength and flexural strength were observed to be nearly equal to that of normal concrete mix. Therefore, use of recycled concrete aggregate showed acceptable performance with respect to mechanical properties. The recycled aggregates obtained from waste concrete are more angular and have higher absorption and specific gravity than natural coarse aggregates and it resulted in increased strength and improved load carrying capacity. However, further studies to determine the effect on durability and improvement on workability are necessary. Keywords: Recycled aggregates, Natural aggregates, Impact test, Static test, First crack and Ultimate failure. 1. INTRODUCTION Concrete is the premier construction material across the world and the most widely used in all types of civil engineering works. Among the ingredients for concrete, aggregates, i.e. inert granular materials such as sand, crushed stone or gravel form the major part. This is mainly because of the running down of quality primary aggregates and greater awareness of environmental protection. Hence the use of recycled aggregate from construction and demolition waste (C&D waste) in concrete is gaining momentum these days. Recycled aggregate concrete may become the need of the day in the years to come. Crushed stone or gravel form the major part. In recent years due to continued large scale extraction, use of aggregates from natural resources has been questioned at international level. 1.1 Literature Review T. Naresh Kumar1, N.Venkata Ramana2, E. Arunakanthi3 and C. Sashidhar4 This paper presents the Behaviour of stone waste aggregate (SWA) concrete slabs under impact loading. The stone waste was obtained during extraction of layered stone (at mines) and at polishing stone industries. This stone waste is converted in useful aggregate and used in the concrete as coarse aggregate in the place of natural aggregate with replacement levels of 0, 25, 50, 75 and 100%. For each replacement level, three slab specimens were cast and tested. 0% replacement level consider as Natural Aggregate Concrete (NAC) slabs. The SWA slabs were compared with natural aggregate concrete (NAC) slabs. The results showed that the SWA slab performance is less than the natural aggregate concrete slabs. From experimental results, regression models were developed to estimate energy absorption at first and ultimate crack stages. In addition to the slab specimens cubes were cast and tested. The cube strength results were used during development of regression models. HardikGandhi1, Dr. DharshanaBhatt2 and Chetnaben Vyas3 studied that There is a critical shortage of virgin aggregates and hence the availability of demolished concrete for use as recycled concrete aggregate (RCA) is increasing. Using the waste concrete as RCA conserves virgin aggregates, reduces the impact on landfills, decreases energy consumption and can provide cost savings. Recycled aggregates are comprised of crushed, graded inorganic particles processed from the materials that have been used in the constructions and demolition debris. Recycled aggregates for application in high strength structural concrete, which will give a better understanding on the properties of concrete with recycled aggregate, as an alternative material to coarse aggregate in structural concrete. In the present study recycled coarse aggregate have been used to replace virgin coarse aggregate. The properties of fresh as well as hardened concrete made of partial/full replacement of recycled coarse aggregate are found out and the results are compared with that of concrete using virgin coarse aggregate.
  • 2. International Research Journal of Engineering and Technology (IRJET) e-ISSN: 2395-0056 Volume: 06 Issue: 10 | Oct 2019 www.irjet.net p-ISSN: 2395-0072 © 2019, IRJET | Impact Factor value: 7.34 | ISO 9001:2008 Certified Journal | Page 500 2. MATERIALS AND METHODOLOGY 2.1 Cement Cement paste is the binder in concrete that holds the aggregate (coarse, fine, micro fine) together and reacts to form hardened mass. The property of concrete depends on the quantities and the quality of its constituents. In this present investigation Ordinary Portland Cement of 53 Grade with a brand name Ultra Tech (Birla Super) used. Tests are conducted in accordance with the Indian standards confirming to IS-12269:1987. The physical characteristic of the tested cement has been shown in table 2.1 Table 2.1: Physical Characteristics of Cement Physical Properties of Cement Test Results Requirements as per IS 12269: 1987 Specific Gravity 3.20 3.15 Fineness of cement 2.83% Less than 10% Standard Consistency 32% Not Specified Soundness (Le- chatelier’s) 0.5mm Shall not be more than 10mm Setting time (in minutes) Initial Setting time 105 Shall not be less than 30 minutes Final Setting Time 510 Shall not be more than 600 minutes Compressive Strength (Mpa) (70.5x70.5x70.5mm ) 3 Days Strength 38.7 MPa Shall not be less than 27.0 MPa 7 Days Strength 48.2 MPa Shall not be less than 37.0 MPa 28 Days Strength 56.8 MPa Shall not be less than 53.0 MPa 2.2 Fine Aggregate HPC contains a large quantity of fine cementations materials. Grading of FA should not cause increase in water demand for concrete. It is desirable to use a coarser variety of sand having high fineness modulus. Both natural sand and crushed stone dust can be used as fine aggregate, should consists of rounded particles to reduce water demand. Generally, fractions passing through 4.75 mm sieves and entirely retained on 150µ sieve are used. Locally obtained manufactured sand was used as the fine aggregate in the concrete mix. The test on fine aggregate was conducted in accordance with IS: 650-1966 & IS: 2386-1968 to determine specific gravity and fineness modulus. Table: 2.2 Physical Characteristics of Fine Aggregate Sl. No. Particular of Test Results 1 Fineness Modulus 2.3 2 Specific Gravity 2.608 3 Bulk Density (kg/m3) Dense rodded 1736 1560 4 Zone II
  • 3. International Research Journal of Engineering and Technology (IRJET) e-ISSN: 2395-0056 Volume: 06 Issue: 10 | Oct 2019 www.irjet.net p-ISSN: 2395-0072 © 2019, IRJET | Impact Factor value: 7.34 | ISO 9001:2008 Certified Journal | Page 501 2.3 Coarse Aggregate Coarse aggregates passing 12.5 mm sieve size and retained on 10 mm sieve were used. The sieve analysis of combined aggregates confirms to the specifications of IS 383: 1970 for well graded aggregates. The tests on the coarse aggregate were conducted in accordance with IS 2386-1963 to determine Specific gravity, Bulk density and Fineness modulus. The results were presented in Table 2.3 Table 2.3: Physical Properties of Coarse Aggregates (12.5mm down size) Sl. No. Particulars Results As Per Is:383-1970 1 Fineness Modulus 4.2 --- 2 Specific Gravity 2.63 --- 3 Bulk Density (Dry-Rodded) 1673 Kg/m3 --- 4 Elongation Index 11% 15% 5 Flakiness 13.8% 15% Crushing Value 24.8% 30% (Max) 7 Impact 17.8% 30% (Max) 8 Los Angeles Abrasion value 29.9% 30% (Max) 2.3 Recycled aggregate concrete (RAC) There are many reasons why concrete has been the most widely used material in the world for many decades now. The most advantageous characteristics of concrete can be listed as: relatively low cost, grand scale availability of its raw components, durability, workability, how adaptable concrete is to be shaped into any form and its fire resistance. But there is a price to pay for all these benefits, namely, the colossal energy consumption and devastating pollution that results from the manufacturing of cement. To reduce this impact and achieve a more sustainable product, waste materials can be incorporated into concrete in the form of RA. The most extensively researched material used in the production of RA is waste concrete, that is, fine and coarse debris from demolition sites. Also, less common components such as glass, coal fly ash, plastic, tyres, volcanic ash and foundry sand have been investigated by several researchers. Concrete with RA as a component in the mixing process is referred to as recycled aggregate concrete. Since aggregates are a vital part of concrete, and concrete is widely used in the world today, this thesis presents a brief literature review on the use of RA in the production of concrete, the end product is referred to as recycled aggregate concrete (RAC). The aim of this review is to establish the mechanical properties of RAC and to compare results with the mechanical performance of conventional concrete, that is, concrete made of aggregates that did not incorporate recycled materials as aggregate. 3. LABORATORY INVESTIGATIONS 3.1 Design of Slabs Table: 3.1The details of the slab design Thickness (mm) Dimension of slab (mm) Main Distribution Length (mm) spacing Mai n Distribution 50 600X600 6 6 550 550 80 mm c/c
  • 4. International Research Journal of Engineering and Technology (IRJET) e-ISSN: 2395-0056 Volume: 06 Issue: 10 | Oct 2019 www.irjet.net p-ISSN: 2395-0072 © 2019, IRJET | Impact Factor value: 7.34 | ISO 9001:2008 Certified Journal | Page 502 3.2 Casting of Slab Specimens This part deals with the casting of reinforced slab specimens. Totally eighteen reinforced concrete slabs were cast and tested, the sizes of the test specimens were selected to suit the capacity of test equipment available in the laboratory. The slabs are designed as two-way slabs by treating as an interior panel (all four sides continuous). The live load considered for this study is 8 kN/m2 and the design is as per IS- 456:2000. The design details of all twelve slabs are as given below in the table. The design of slabs in detail are shown in above table 3.1. All slabs were (600 X 600) mm with thickness of 50 mm. All the slabs were designed as two-way slabs. The tensile reinforcement ratio varied according to the thickness of slabs. The clear cover to reinforcement was 15 mm on all faces. The typical details of the pattern of the reinforcement and cross section of the slabs are shown in Fig 3.6. Totally twelve (six for static test and six for impact test) test slab specimens are named sequentially as CS, CS + 10%, CS + 20%, CS + 30%, CS+40%, CS+50% were casted. After 24 hours, test specimens were demolded and the test specimens were cured continuously for 28 days. Details of Slabs are given below. Totally twelve (six for static test and six for impact test) test slab specimens are named sequentially as CS, CS + 10%, CS + 20%, CS + 30%, CS+40%, CS+50% were casted. After 24 hours, test specimens were demolded and the test specimens were cured continuously for 28 days. Details of Slabs are given below Slno Slabs No of Specimens 1 M30 2 2 M30+10%RCA 2 3 M30+20%RCA 2 4 M30+30%RCA 2 5 M30+40%RCA 2 6 M30+50%RCA 2 3.3 Casting of Cubes and Prisms 3.3.1 Casting of cubes (150*150*150mm) and prisms (100*100*500mm)  Initially moulds are cleaned and oiled. The next step involved fixing the mould end plates using nuts and bolts.  Weigh the amount of cement, silica fume, GGBS, fine aggregates and coarse aggregates for moulds. Materials were first dry mixed, then mixed with 1/3rd amount of total water with super plasticizer and polypropylene and steel fibre are added to M30 concrete. Remaining water was then added and mixed thoroughly to get homogeneous mix.  Then the mould was fully compacted by using the vibrating machine. Sufficient care was taken to see that concrete was properly filled in corners and the edges of the mould. As soon as the air bubbles stopped to rise, the top surface of the mould was finished with trowel by applying little pressure. 3.3.2 Curing After 24 hrs concrete specimen are removed from the moulds and kept for curing in water bath for the required days of curing. All Specimens are cured for 3 days, 7 days & 28 days as per standard procedure.
  • 5. International Research Journal of Engineering and Technology (IRJET) e-ISSN: 2395-0056 Volume: 06 Issue: 10 | Oct 2019 www.irjet.net p-ISSN: 2395-0072 © 2019, IRJET | Impact Factor value: 7.34 | ISO 9001:2008 Certified Journal | Page 503 4. MECHANICAL PROPERTIES Testing of hardened concrete place an important role in controlling and confirming the quality of cement concrete works. Systematic testing of raw materials, fresh concrete and hardened concrete are inseparable part of any quality control program for concrete which helps to achieve higher efficiency of the material used and greater assurance of the performance of concrete with regard to both strength and durability. One of the purposes of testing hardened concrete is to confirm that the concrete used at site has developed the require strength. As the hardening of concrete takes time one will not come to know the actual strength of concrete for some time. Tests are made by casting cubes or cylinders from the representative concrete or cores cut from the actual concrete. 4.1 Compressive strength The compressive strength of concrete i.e. ultimate strength of concrete is defined as the load which causes failure of the specimen divided by the area of the cross section in unit- axial compression, under a given rate of loading i.e., 13.73 N/mm2. To avoid large variation in the results of compression test, care should be taken during the casting of the test specimens and loading as well. The cube mould of 150mm x 150mm x 150mm size is taken as per IS: 516-1959 specification. The cubes were tested in 200T capacity compressive testing machine. Place the specimen in the machine then apply the load continuously, uniformly and without shock. The rate of loading is continuously adjusted in Newton’s through rate control valve by hand. The load is increased until the specimen fails and record the maximum load carried by specimen during the test. Fig 1 shows the testing of cube specimen in progress. The compression strength is calculated using the formula, f = P/A Where, f = is compressive strength of concrete in N/mm2 P = ultimate load resisted by concrete Fig.1. Compressive testing of Cubes 4.2 Flexural strength Flexural strength is expressed in terms of “Modulus rupture” which is the maximum tensile (or compressive) stress at rupture. Modulus of rupture Modulus of rupture is defined as the normal tensile stress in concrete, when cracking occurs in a flexure test. This tensile stress is the flexural strength of concrete and is calculated by the use of the formula, which assumes that the section is homogeneous. fb = (p x l) / (b x d2) Where,
  • 6. International Research Journal of Engineering and Technology (IRJET) e-ISSN: 2395-0056 Volume: 06 Issue: 10 | Oct 2019 www.irjet.net p-ISSN: 2395-0072 © 2019, IRJET | Impact Factor value: 7.34 | ISO 9001:2008 Certified Journal | Page 504 fb = modulus of rupture, N/mm2 b = measured width in mm of the specimen d = measured depth in mm of the specimen at the point of failure l = length in mm of the span on which specimen was supported p = max. Load in N applied to the specimen  Prisms are tested immediately on removal from the water while they are still in wet condition. The bearing surfaces of the supporting and loading rollers are wiped clean, and loose sand or other material removed from the surfaces of specimen where they are to make contact with the rollers. The specimen is then placed in the machine in such a manner that the load is applied to the uppermost surface as cast in the mould, along two lines spaced 13.3cm apart (If the fracture occurs within the middle third of the span, a>133mm, fb = pl/bd2.  If the fracture occurs outside the middle third but deviating by not more than 5 percent of the span length, 110<a<133mm Then, fb = 3PL/bd ² Where, P= Load L = span in mm a= distance between line of fracture and the nearest support in mm b = average breadth of the specimen in mm d = average depth of the specimen in mm If fracture occurs by more than 5 percent outside the middle third, a<110mm, then the results of the test should be rejected. Fig. 2. Flexural Test on Beam Prisms 5. STATIC TESTING OF SLABS 5.1 General  A static test setup is fabricated for the test programme, which should have relatively stiff supports and the hydraulic loading assembly is fixed to the supporting frame. Since the study is mainly aimed at evaluation of static
  • 7. International Research Journal of Engineering and Technology (IRJET) e-ISSN: 2395-0056 Volume: 06 Issue: 10 | Oct 2019 www.irjet.net p-ISSN: 2395-0072 © 2019, IRJET | Impact Factor value: 7.34 | ISO 9001:2008 Certified Journal | Page 505 response due to load, as also the cumulative effect of such loading on the concrete slab elements, a hydraulic jack type loading has been employed for Static Testing Machine.  The static testing machine used in the present investigation is of hydraulic loading type instrumented assembly. The detailed view of the above machine is shown in Fig. 3. Fig. 3. Static Test Setup 5.2 Instrumentation The following instrumentation is used in the present experimental investigation to study the behaviour of the slabs under static loading. This consists of two Linear Variable Differential Transducers (LVDT), one at center and another at quarter span and are used to receive displacement variation with time. Load cell attached to the head of the hydraulic jack to record load time history. From the literature review it has been observed that a single assembly of instrumentation was not possible. The incorporation of electronic devices to record the specimen response to different energy level of impact is proved to be very efficient hence the data acquisition system along with LVDT, accelerometer and load cell is essential. In the present investigation the dynamic response and other parameters are studied with the help of very sensitive electronic devices. The response send by these devices are analyzed through a software programme to get actual experimental values. In addition, the data Acquisition system are used in the present investigation. 5.3 LVDT LVDT (Linear Variable Different Transformer) is a sensitive device, shown in fig 4. used for measuring minute mechanical displacements. It consists of LVDT coil Prising of primary and two secondaries wound on an acrylic bobbin. A ferromagnetic core moves inside the coil. The output is proportional to the displacement. The electric inputs/outputs are termed on to a 6 – pin MS connector. Fig. 4. LVDT and its Fixtures
  • 8. International Research Journal of Engineering and Technology (IRJET) e-ISSN: 2395-0056 Volume: 06 Issue: 10 | Oct 2019 www.irjet.net p-ISSN: 2395-0072 © 2019, IRJET | Impact Factor value: 7.34 | ISO 9001:2008 Certified Journal | Page 506 5. IMPACT TESTING OF SLABS 5.1 General Since the study is mainly aimed at evaluation of dynamic response due to load, as also the cumulative effect of such blows on the concrete slab elements, impact test a low velocity drop weight has been employed in the present experimental investigation. The main objective of this investigation is to study the load-time variation, displacement-time variation and energy absorption capacity of slabs under low velocity repeated impact loading. Such data obtained from tests are to be analyzed to study the behaviour of slab under low velocity repeated impact loading. 5.2 Impact Testing Machine The impact testing machine used in the present investigation is of low velocity drop weight type instrumented impact testing machine: The detailed view above machine is shown in Fig 5. The impact testing machine consists of major three parts are as follows. In impact test the impact load was applied by means of the free fall of a drop weight from 1m height. For free fall the drop weight was arranged, to fall between the guided cylinder and impact the specimen at midpoint. The drop weight had a steel circular load cell of diameter 5.5cm as shown in the fig below. Fig.5. Impact Test Setup 5.3 Instrumentation The following instrumentation is used in the present experimental investigation to study the impact behaviour of the slabs under low velocity drop weight impact loading. This consists of,  Two Linear Variable Differential Transducers (LVDT), one at center and another et quarter span and are used to receive displacement variation with time  An accelerometer are used for recording acceleration time history.  Load cell attached to the head of striker to record load time history Fig. 6. Drop Hammer
  • 9. International Research Journal of Engineering and Technology (IRJET) e-ISSN: 2395-0056 Volume: 06 Issue: 10 | Oct 2019 www.irjet.net p-ISSN: 2395-0072 © 2019, IRJET | Impact Factor value: 7.34 | ISO 9001:2008 Certified Journal | Page 507 From the literature review it has been observed that a single assembly of instrumentation was not possible. The incorporation of electronic devices to record the specimen response to different energy level of impact is proved to be very efficient hence the data acquisition system along with LVDT, accelerometer and load cell is essential. In the present investigation the dynamic response and other parameters are studied with the help of very sensitive electronic devices. The response sends by these devices are analyzed through a software programmed to get actual experimental values. In addition, the data Acquisition system are used in the present investigation. 6. TEST RESULTS AND DISCUSSION OF EXPERIMENTAL PROGRAMME 6.1 Compression Test on Standard Cubes The test is conducted as per IS: 516-1959 (Reaffirmed 2008). The experimental compressive strength values obtained on standard cube specimen of size 150 mm x 150 mm x 150 mm, cured for 7 days and 28 days for all four different concrete matrices are presented in the form of graphs and bar charts shown in figure. Compressive Strength DAYS M30 M30+10%RCA M30+20%RCA M30+30%RCA M30+40%RCA M30+50%RCA 7 26.37 22.55 24.33 21.77 20.11 18.85 28 34.66 26.03 28.43 24.66 22.88 21.55
  • 10. International Research Journal of Engineering and Technology (IRJET) e-ISSN: 2395-0056 Volume: 06 Issue: 10 | Oct 2019 www.irjet.net p-ISSN: 2395-0072 © 2019, IRJET | Impact Factor value: 7.34 | ISO 9001:2008 Certified Journal | Page 508 6.2 Static Test Results for Slabs Combined graph of all Specimens 0 5 10 15 20 25 0 2 4 6 8 Load(Kn) Deflection (mm) Load v/s Deflection M30+30%RCA 0 2 4 6 8 10 12 14 16 18 0 2 4 6 8 Load(Kn) Deflection (mm) Load v/s Deflection M30+50%RCA
  • 11. International Research Journal of Engineering and Technology (IRJET) e-ISSN: 2395-0056 Volume: 06 Issue: 10 | Oct 2019 www.irjet.net p-ISSN: 2395-0072 © 2019, IRJET | Impact Factor value: 7.34 | ISO 9001:2008 Certified Journal | Page 509 6.3 Impact Test Results for Slab 7. CONCLUSION In this study it is found that there is not much variation in strength between ordinary concrete and 20% replaced aggregate concrete, which proves the previous works. But when the percentage of aggregate replaced increases there is a constant increase in strengths, which is a controversy to the previous works. Because it has been found that recycled aggregates obtained from recycling concrete are more angular and have higher absorption and specific gravity than natural coarse aggregates it may result on increase of strength and improved load carrying capacity. However, further studies to determine the effect on durability and improvement on workability are necessary. REFERENCES [1] Tomas U. Ganiron Jr, (2015), “Recycling Concrete Debris from Construction and Demolition Waste”, International Journal of Advanced Science and Technology Vol.77, pp.7-24. [2] Roz-Ud-Din Nassar and Previz Soroushian, (2012), “Strength and durability of recycled aggregate concrete containing milled glass as partial replacement for cement”, Construction and Building Materials, Vol. 29. pp. 368–377 [3] Markandeya Raju Ponnada1 and Kameswari P, (2015), “Construction and Demolition Waste Management – A Review”, International Journal of Advanced Science and Technology, Vol. 84, pp.19-46. [4] Jitender Sharma and Sandeep Singla, (2014), “Study of Recycled Concrete Aggregates” `, International Journal of Engineering Trends and Technology (IJETT), Vol. 13, No. 3, pp. 123 – 125. 0 1 2 3 4 0 1 2 3 4 5 0 5 10 15 Displacementmm NO OF Blows ALL SPECIMENS M30+1 0%RCA M30+2 0%RCA M30+3 0%RCA M30+4 0%RCA