SlideShare a Scribd company logo
Problem Cases in the Pressroom
1
Contents
• Electrostatic Charge on Paper
• Crease Formation
• Picking
• Emulsification
• Ghosting
• Mottling
• Horizontal Stripes
• Darkening
• Decrease in Tone Value
• Increase in Tone Value
• Slurring
• Lags in Drying Time
3
Electro Static
Charge on Paper
Printers are familiar with the problem: Printing sheets stick
together because
they are electro-statically charged. The result: Several sheets are
simultaneously
sucked in from the stack, stopping up the feeder. Static electricity
arises from
Either an electron deficit (positive charge) or an excess of
electrons (negative
charge) on the surface of the paper.
An electrostatic charge is especially likely to occur when paper
that is too
dry is processed under conditions of low atmospheric humidity.
The critical
lower limit – as much for paper dampness as for relative humidity
– ranges
from 40 % to 42 %. (Electrostatic = immobile, i.e. static electricity
4
The moisture content of paper should range
between 45 % and 55 %. The electrical conductivity
of paper, and consequently electrical run off,
increases with increasing moisture content.
Working spaces should be air-conditioned or
humidified at a 50 % to 55 % level of relative
humidity. Particularly during colder times of the
year in heated rooms, the atmospheric humidity can
sink dramatically.
Antistatic equipment such as discharge electrodes
and ionic blowers reduce electrostatic charge;
ionization equipment raises the surrounding air’s
electronic conductivity, thereby preventing the build
up of static
charge.
Remedy
During printing, creases are often generated on paper that is poorly
air-conditioned, or does not lie in a flat plane, as well as from paper that
is wavy-edged, baggy-centered, or statically charged. Incorrect settings
on the sheet-feeder or during paper transfer may also lead to the formation
of creases. In order to ensure that the printing stock during the printing
process lies flat, it should be kept properly air-conditioned during storage
and transport. Paper is very sensitive to fluctuations in humidity. This is
why one must be careful to maintain atmospheric humidity and temperature
at constant levels during storage. Paper should demonstrate a relative
humidity from 50 % to 55 %; the temperature should be constant between
20 °C and 22 °C (68 °F and 71.6 °F).
Crease Formation
6
Should creases develop, this may also be the fault of incorrect machine
settings – most likely on the sheet-feeder. Among the reasons creases may
form are incorrectly set or jamming front lays, side lays that draw with too
much force, a hold-down device that has been set too tightly, or an air-blast
that is too strong. An incorrect air-pressure setting at the point of sheet
transfer may also contribute to the formation of creases. Further sources
include poorly functioning or dirty grippers, which warp the sheet, as well
as a printing pressure between the rubber and the impression cylinder
that is set too high, or is uneven. This tumbles the sheet, and will result
in creasing.
…Continued
Remedy
•Employ printing stock that is good and flat
• Inspect the front lays
• Inspect the side lays
• Do not set the hold-down device too tightly
• Reduce the air-blast on the sheet-feeder
• Optimize the air-pressure adjustments at the point of sheet transfer
• Optimize the print lateral feed
• Inspect, clean, and adjust the grippers as needed
Picking occurs when small particles are
torn out of the surface of the paper, or
printing stock rips during the printing
process. This can cause damage to the
printing blanket. It becomes necessary to
wash more frequently, and print quality is
adversely affected.
Picking becomes a problem when surfaces are not
sufficiently resilient. This
indicates that the tractive force of the printing ink is greater
than the fiber
adhesion in the paper structure, or the bonding of the
pigment used in the
coating. Inadequate gluing, or the poor anchoring of the
coating material on
the paper’s surface may cause picking
Picking
Remedy
• Employ a soft series of inks
• Reduce the ink’s tractive force (add printing oil)
• Allow the machine to run on standard working condition
• Raise the rasp temperature (temper the inking system)
• Reduce the speed of the machine; this lessens the traction on the
paper
• Use a quick release blanket
• Employ paper of better quality
Emulsification
Emulsion is a mixture of ink and dampening solution. In this process,
Dampening solution is distributed evenly throughout the ink in small droplets.
The proportion of water in a “stabile emulsion” is around 20 %. If
higher, then the ink’s splitting properties are reduced, and the ink flow is
interrupted. As a result, the emulsion becomes unstable, the ink “builds
up”, and it “emulsifies”. Too large a proportion of dampening solution in
the printing ink, or too low a pH-value fosters emulsification. Printing inks
react differently, depending on what type they are: blended inks, dayglo,
or metallic inks are more sensitive than inks in the normal scale. Emulsified
printing inks will increase drying times, as well as increasing the risk
of deposits.
Remedy
• Set the ink and dampening balance correctly, and check on it continuously
throughout the printing process.
• In case of emulsified ink, wash the rollers, and re-establish the
smearing limit.
• Check the dampening solution, and change it regularly (the ideal
dampening
solution has a water hardness from 8 to 12° dH, a pH-value
from 4.8 to 5.5, and a temperature from 10 °C to 15 °C (50 °F to 59 °F).
• On an Alcolor dampening unit: separate the intermediate roller from
the inking unit; install cross-flow ventilators.
• Avoid frequent phases of pre- and post-dampening (during make-ready
or stoppages).
• Inspect and optimize the adjustment of the inking and dampening rollers.
• Where there is less ink taking, an additional ink stripe may be introduced
to stabilize the balance of ink and water
Ghosting
By ghosting, one understands a circumstance where
printing form elements other than the desired positive
or negative ones duplicate themselves onto the printed
surface. These “stencils” or “ghost images” emerge
from repeated passes of the ink form roller over the plate
cylinder, and from a reduction or accumulation of ink. Used (hard) or
poorly
adjusted ink-rollers facilitate ghosting, and the tendency toward ghosting
increases with weak pigment inks. An optimal balance between ink and
dampening solution helps prevent ghosting, since too much water
negatively
influences printing outcomes.
Remedy
• When maintaining rollers, only use the appropriate cleansing agents;
a weekly application of wash paste removes lime deposits, and will
regenerate the rollers.
• Adjust the rollers in accordance with the instruction manual; inspect
the adjustment regularly.
• Change used rollers: the rubber surface of older rollers will become glossy
and over-smooth. At the same time, as their hardness increases, the edges
bulge out in a trumpet shape. More pronounced abrasion becomes evident.
• Adjust for maximum lateral distribution.
…Continued
• Adjust reciprocation of the ink form rollers
• Shift the engaging point of the lateral distribution
• Reduce the quantity of dampening solution being used (smearing
limit)
• Employ high pigment inks
• Turn on the vario
• Turn the printing form (prepress)
Mottling
When speaking of “mottling” or “back trap mottling“, printers are referring
to a cloudy print output. The problem originates in paper that is partially
uneven, and the resulting uneven absorption and back split characteristics.
If the paper is spotted, or if a certain amount of cloudiness is already present
in the coating, then the printing ink will be only partly absorbed. In 4-color
Sheetfed offset printing, the printing result will back split on the printing
blankets of the subsequent printing units. When an uneven penetration of
printing ink is especially pronounced, this will become visible after the back
split process occurs, as an uneven print reproduction. The problem of a
“cloudy printout” manifests itself in the greatest variety in offset printing.
In order to isolate the printing paper as the culprit, one must first determine
if the visual appearance of the cloudy printout matches up with the paper
structure. This can be done using backlighting, or under UV light. The absorption
characteristics of the printing ink on the paper in question can also be
made visible by resorting to a simple wipe test using special wipe-test ink.
In this way, the proof that paper is the root cause may be adduced.
Remedy
In cases where the cloudy printout is purely the result of the
paper being used, the only solution is to change to an
alternative type of paper.
Horizontal Stripes
The problem in this case involves disturbances in the printed image, which
are manifested as bright or dark stripes running horizontally to the direction
of printing. Horizontal stripes arise for a variety of reasons. Besides adjustment errors,
errors in screen vignettes (prepress errors) may also play a role. Additionally,
the formation of stripes may also be influenced by contamination from the
build up of powder and coating, from damage to the printing blanket or the
printing plate, or from the ink/dampening solution feeds, as well as from
the quality of the ink. The machines themselves may also be causing the
stripes, for example from an incorrect alignment of the ink and dampening
units, or from rolling errors (too much pressure). Tone stripes can be caused
by the relative lateral movement of the rollers on the printing plate.
Remedy for stripe formation
conditioned by machines
• When maintaining the rollers, only use appropriate cleansing agents;
the weekly application of a wash paste removes lime deposits, and will
regenerate the rollers.
• Adjust the rollers in accordance with the instruction manual; inspect the
adjustment regularly.
• Change used rollers: the rubber surface of older rollers becomes glossy
and over-smooth. At the same time, as their hardness increases, the
edges bulge out in the shape of a trumpet. More pronounced abrasion
becomes evident.
• Adjust reciprocation of the ink form rollers
• The dampening distributing cylinder must be kept clean and receptive to
water.
• The roll bearings must be in fine working condition (no play, no sticking).
• Lubricate the roll bearings.
…Continued
• By setting the ink form rollers as gently as possible on the printing
plate,
impacts stemming from the run-on and run-off edges are reduced.
• The bearer ring should be kept clean and grease-free.
• The calibrated underpacking should be clean, cut in a format to fit, and
correctly inserted.
• Clamping between the plate and the blanket should range between
0.1 mm and a max. 0.13 mm. (0.004 in and 0.051 in).
• Clamping between the blanket and the counterpressure should be set
in consideration of the surface of the printing stock; avoid clamping that
is set too high.
Darkening
When darkening occurs, the darker colors are transferred from the blanket
over the printing plate onto the succeeding inking system, where they
contaminate
the light colors.
During wet-on-wet printing, the tackiness of the inks must be coordinated.
Nevertheless, it can happen that the darker colors from the first
printing units contaminate the lighter colors (mainly yellows) in the latter
printing units.
original
tone color after
blanket
contamination
Remedy
• Change to a different kind of ink
• Deposit the lighter colors more in the direction of the sheet-feeder.
• Follow the rule of thumb “screen before surface” for the inking
sequence.
• Raise the dampening solution feed in the lighter colors, or increase
the lighter colors.
Decrease in Tone Value
The reduction of the halftone dot in the print
when compared to the original (film, printing
plate) is referred to as a decrease in tone value.
This phenomenon may already arise in
prepress.
In addition, various parameters
can also have a bearing on abrasion of the
printing plate:
• Normal plate wear and tear
• Coating build up or powder deposits on the blanket
• Unsuitable plate cleanser (admixture of abrasive material)
…Continued
• A pH-value in the dampening solution that is too low may slightly etch
the edges of the halftone dots.
• An alcohol content that is too high corrodes the ink-accepting coating.
• Rapidly volatizing cleansing solutions may damage the printing plate.
Remedy
• Employ appropriate printing plates
• Use a suitable plate cleanser and certified cleaning solution when
Maintaining the printing plate.
• Avoid using abrasive powder (calcium carbonate)
• Always prepare dampening solution according to instructions (pH-value,
alcohol concentration); the ideal dampening solution has a water hardness
of 8 to 12° dH, a pH-value of 4.8 to 5.5, and a temperature
Ranging from 10 °C to 15 °C (50 °F to 59 °F).
Increase in Tone Value
An increase in tone values means a gain in the halftone dot of the print
compared to the original (film, printing plate). In order to establish an increase
in tone value, a full tone field combined with a defined grid is needed. The
problem of an increase in tone value may already arise during the preparation
of the printing form. While an increase in tone value in a printing press
cannot be entirely avoided, it should never be allowed to exceed a certain
point. An increase in tone value depends on type of ink, ink quantity, the
temperature in the inking system, the surface of the printing stock, the
clamping, the blanket type, the dampening solution, and the quantity of
dampening solution employed.
Remedy
• Print with a familiar ink series, if possible without additives, within the
tolerance levels of your own standards of density.
• An increase in tone value (approx. 2 %) must be taken into consideration
during black and white printing.
• Employ appropriate black and white inks
• Set the inking system between 27 °C and 30 °C (80 °F and 86 °F)
• Avoid changing the printing stock during the print run
…Continued
• Clamping between the plate and the blanket should be set between
0.1 mm and max. 0.13 mm (0.004 in and 0.051 in)
• Pressing between the blanket and the counterpressure should be set
to reflect the printing stock surface; avoid setting compression too high.
• A fixed type of blanket should be used in the pressroom
(standardization)
• Only use certified cleansing solutions when washing.
• Wash new blankets with water after mounting in order to remove
the talcum.
• Newly stretched blankets must be restretched.
• Run the quantity of dampening solution slightly over the smear limit, and
precisely maintain the balance of ink and dampening solution.
• Optically test the three-quarter tones with a line tester.
% TWZ for CMY
including tolerances
TWZ for K
including tolerances
40 13,0 +/– 3 16,0 +/– 3
50 14,3 +/– 3 17,0 +/– 3
70 13,4 +/– 3 14,9 +/– 3
80 10,7 +/– 3 11,5 +/– 3
ISO Standard Values
Slurring
One speaks of slurring when the geometry of the halftone dot changes. The
printed image then appears to be displaced. The round halftone dot
assumes an oval shape. Two types of slurring exist – on the one hand, in the
direction of printing (circumferential slurring), and on the other hand,
transverse to the direction of printing (lateral slurring). These effects lead to a
reduction in quality, and reflect the processing conditions within the group
comprising the plate, blanket, and printing cylinders, as well as on other
material influences.
Remedy
• Check the printing pressure adjustment, and reduce as needed
• Maintain recommended packing thicknesses (control with a
cylinder gauge)
• Mount the blankets carefully, and use a torque wrench when stretching
• Insert the blankets in the printing press in the indicated weave direction
• Clean the grippers and adjust them as needed
Lags in Drying
If the ink dries too slowly in the stack, one speaks of a lag in drying time.
This may lead to an ink rub-off of the print during print finishing or
during transport. The interaction between ink, additives, and dampening
solution is usually to blame for lags in drying time. For example, should the
pH-value of the dampening solution fall below 4.7, one can count on a
longer drying time. Incorrectly dosed additives (drying accelerators), a stack
temperature that is too low, or excessively emulsified ink also retards
drying. In principle, the heavier the ink film, the slower the drying process.
Remedy
• Optimal tuning between ink and paper (inquire with the manufacturer)
• Do not allow the pH-value of the dampening solution to cross below 4.7
• Avoid ink emulsification
• Only dose additives according to the manufacturer’s indications
• In cases of lower ink taking, also print ink stripes
• Avoid high ink film densities (employ ink reduction or high pigment
inks)
• Use IR drying
• In order to rescue a print job, coat it with an oil or dispersion varnish
33
Contact Us
Mr. Rajendra Prasad.
Rajendra.prasad@heidelberg.com
www.heidelberg.com
Copyright © 2014 Heidelberg India, All rights reserved.
Heidelberg India Keeps members of Printing industry informed
About its latest development and attractive offers.
Problem cases in press rooms

More Related Content

PDF
Printing technology : problems sheetfed offset
PDF
Formation of Print
PPT
Print quality
PPTX
How offset printing works
PPTX
Delamination in sheetfed offset printing
PPTX
Offset printing
PPS
Flexographic printing 1(9551)
PPTX
Problem Cases in the Pressroom
Printing technology : problems sheetfed offset
Formation of Print
Print quality
How offset printing works
Delamination in sheetfed offset printing
Offset printing
Flexographic printing 1(9551)
Problem Cases in the Pressroom

What's hot (20)

PPTX
Pro printing
PPT
Flexografia
PPT
Basics of offset printing and other printing techniques
PPTX
Scratches on Folding Box Packaging
PPTX
Printing techniques
PDF
Printing technologies compared
PPTX
FlexografíA
PPTX
The printing processes
PDF
Mottling in offset printing
PPTX
Flexography
PPTX
Different types of printing techniques
PDF
PPT
Modern printing technologies
PPTX
Modern Printing Technology
PPT
Computer to Plate - Presentation
PPSX
PDF
TECNICAS DE IMPRESION
PPT
Nm rotogravura
PPTX
Las tintas de impresión
 
PDF
What is offset printing
Pro printing
Flexografia
Basics of offset printing and other printing techniques
Scratches on Folding Box Packaging
Printing techniques
Printing technologies compared
FlexografíA
The printing processes
Mottling in offset printing
Flexography
Different types of printing techniques
Modern printing technologies
Modern Printing Technology
Computer to Plate - Presentation
TECNICAS DE IMPRESION
Nm rotogravura
Las tintas de impresión
 
What is offset printing
Ad

Viewers also liked (16)

PPTX
Dampening Solutions in Offset Printing
PPT
Printing technology sheetfed offset (1)
PPTX
Ink and dampening solution in balance 1
PPT
How offset printers work
PPTX
Neeraj Presentation
PPTX
Heidelberg Tips & Tricks- Ink & Dampening Solution in Balance.
PPTX
нүүр амны эмчилгээний үед хийгдэх физик эмчилгээ
PDF
Printing processes
PDF
Carbonless Fountain Solutions/PH
PPTX
Slides on avoiding ghosting
PPTX
Avoid ghosting
PPTX
Slides on avoiding ghosting
PPTX
Slides on ink dampening solutions in bal 2
PDF
Ghosting and vanishing dots in heatset printing
PPT
Print defects in heatset
PDF
Siegwerk Nutriflex 10 slideshare oct 2016
Dampening Solutions in Offset Printing
Printing technology sheetfed offset (1)
Ink and dampening solution in balance 1
How offset printers work
Neeraj Presentation
Heidelberg Tips & Tricks- Ink & Dampening Solution in Balance.
нүүр амны эмчилгээний үед хийгдэх физик эмчилгээ
Printing processes
Carbonless Fountain Solutions/PH
Slides on avoiding ghosting
Avoid ghosting
Slides on avoiding ghosting
Slides on ink dampening solutions in bal 2
Ghosting and vanishing dots in heatset printing
Print defects in heatset
Siegwerk Nutriflex 10 slideshare oct 2016
Ad

Similar to Problem cases in press rooms (20)

PPTX
Flexo Troubleshooting.pptx
PPTX
AQUEOUS FILM COATING AND PROCESS PARAMETERS
PPTX
Defects or processing problems in tablet dosage form.
PPTX
Defects or processing problems in tablet dosage form.
PPTX
tablet defect causes.pptx
PPTX
Heidelberg Tips & Tricks - Printing with Uncoated Paper
PDF
Jon-Porter-Mejores-prácticas-en-corrugadoptimize.pdf
PPTX
Tablet processing problems and its remedies for poster presemntation
PPTX
Coating Not Cracking
PPTX
Surface sizing of paper which enahnces the surface properties of the paper
PPTX
Processing problems in tablet manufacturing
PPTX
Processing problems in tablet manufacturing
PPTX
Devanu n ishan
PPTX
Viscosity
PPS
Stallion - Thermal Printer - Print Head
PPTX
Tips & Tricks: Paper Problems – Combating Static Electricity & Creasing
PDF
Heidelberg roller setting
PPT
Finishing defects
PPTX
Heidelbergpresentation - coating
PDF
Tableting compression challenges with solutions
Flexo Troubleshooting.pptx
AQUEOUS FILM COATING AND PROCESS PARAMETERS
Defects or processing problems in tablet dosage form.
Defects or processing problems in tablet dosage form.
tablet defect causes.pptx
Heidelberg Tips & Tricks - Printing with Uncoated Paper
Jon-Porter-Mejores-prácticas-en-corrugadoptimize.pdf
Tablet processing problems and its remedies for poster presemntation
Coating Not Cracking
Surface sizing of paper which enahnces the surface properties of the paper
Processing problems in tablet manufacturing
Processing problems in tablet manufacturing
Devanu n ishan
Viscosity
Stallion - Thermal Printer - Print Head
Tips & Tricks: Paper Problems – Combating Static Electricity & Creasing
Heidelberg roller setting
Finishing defects
Heidelbergpresentation - coating
Tableting compression challenges with solutions

More from Heidelberg India (15)

PPTX
Slides on delamination
PPTX
S.prst on color measurement the right way....
PPTX
Slides on coating not cracking
PPTX
Slides on printing with uncoated paper
PPTX
Slides on environmentally friendly
PPTX
Foggy film laminated prints
PPTX
Perfect plate production seeing the light!
PPTX
Block printing tips and tricks
PPTX
Inking roller
PPTX
Regular maintenance
PPTX
Key to good offset printing
PPTX
Drying Systems
PPTX
Color management
PPTX
Heidelberg presentation -Color Measurement
PPTX
Heidelberg presentation
Slides on delamination
S.prst on color measurement the right way....
Slides on coating not cracking
Slides on printing with uncoated paper
Slides on environmentally friendly
Foggy film laminated prints
Perfect plate production seeing the light!
Block printing tips and tricks
Inking roller
Regular maintenance
Key to good offset printing
Drying Systems
Color management
Heidelberg presentation -Color Measurement
Heidelberg presentation

Recently uploaded (20)

PPTX
KOM of Painting work and Equipment Insulation REV00 update 25-dec.pptx
PDF
Dropbox Q2 2025 Financial Results & Investor Presentation
PPTX
Effective Security Operations Center (SOC) A Modern, Strategic, and Threat-In...
PDF
Architecting across the Boundaries of two Complex Domains - Healthcare & Tech...
PDF
The Rise and Fall of 3GPP – Time for a Sabbatical?
PPT
Teaching material agriculture food technology
PDF
NewMind AI Weekly Chronicles - August'25 Week I
PDF
Empathic Computing: Creating Shared Understanding
PPTX
20250228 LYD VKU AI Blended-Learning.pptx
PPTX
Cloud computing and distributed systems.
PDF
KodekX | Application Modernization Development
PDF
Machine learning based COVID-19 study performance prediction
PDF
Agricultural_Statistics_at_a_Glance_2022_0.pdf
PDF
Profit Center Accounting in SAP S/4HANA, S4F28 Col11
PDF
cuic standard and advanced reporting.pdf
PDF
Per capita expenditure prediction using model stacking based on satellite ima...
PDF
Peak of Data & AI Encore- AI for Metadata and Smarter Workflows
PDF
Diabetes mellitus diagnosis method based random forest with bat algorithm
PDF
Chapter 3 Spatial Domain Image Processing.pdf
PDF
Optimiser vos workloads AI/ML sur Amazon EC2 et AWS Graviton
KOM of Painting work and Equipment Insulation REV00 update 25-dec.pptx
Dropbox Q2 2025 Financial Results & Investor Presentation
Effective Security Operations Center (SOC) A Modern, Strategic, and Threat-In...
Architecting across the Boundaries of two Complex Domains - Healthcare & Tech...
The Rise and Fall of 3GPP – Time for a Sabbatical?
Teaching material agriculture food technology
NewMind AI Weekly Chronicles - August'25 Week I
Empathic Computing: Creating Shared Understanding
20250228 LYD VKU AI Blended-Learning.pptx
Cloud computing and distributed systems.
KodekX | Application Modernization Development
Machine learning based COVID-19 study performance prediction
Agricultural_Statistics_at_a_Glance_2022_0.pdf
Profit Center Accounting in SAP S/4HANA, S4F28 Col11
cuic standard and advanced reporting.pdf
Per capita expenditure prediction using model stacking based on satellite ima...
Peak of Data & AI Encore- AI for Metadata and Smarter Workflows
Diabetes mellitus diagnosis method based random forest with bat algorithm
Chapter 3 Spatial Domain Image Processing.pdf
Optimiser vos workloads AI/ML sur Amazon EC2 et AWS Graviton

Problem cases in press rooms

  • 1. Problem Cases in the Pressroom 1
  • 2. Contents • Electrostatic Charge on Paper • Crease Formation • Picking • Emulsification • Ghosting • Mottling • Horizontal Stripes • Darkening • Decrease in Tone Value • Increase in Tone Value • Slurring • Lags in Drying Time
  • 3. 3 Electro Static Charge on Paper Printers are familiar with the problem: Printing sheets stick together because they are electro-statically charged. The result: Several sheets are simultaneously sucked in from the stack, stopping up the feeder. Static electricity arises from Either an electron deficit (positive charge) or an excess of electrons (negative charge) on the surface of the paper. An electrostatic charge is especially likely to occur when paper that is too dry is processed under conditions of low atmospheric humidity. The critical lower limit – as much for paper dampness as for relative humidity – ranges from 40 % to 42 %. (Electrostatic = immobile, i.e. static electricity
  • 4. 4 The moisture content of paper should range between 45 % and 55 %. The electrical conductivity of paper, and consequently electrical run off, increases with increasing moisture content. Working spaces should be air-conditioned or humidified at a 50 % to 55 % level of relative humidity. Particularly during colder times of the year in heated rooms, the atmospheric humidity can sink dramatically. Antistatic equipment such as discharge electrodes and ionic blowers reduce electrostatic charge; ionization equipment raises the surrounding air’s electronic conductivity, thereby preventing the build up of static charge. Remedy
  • 5. During printing, creases are often generated on paper that is poorly air-conditioned, or does not lie in a flat plane, as well as from paper that is wavy-edged, baggy-centered, or statically charged. Incorrect settings on the sheet-feeder or during paper transfer may also lead to the formation of creases. In order to ensure that the printing stock during the printing process lies flat, it should be kept properly air-conditioned during storage and transport. Paper is very sensitive to fluctuations in humidity. This is why one must be careful to maintain atmospheric humidity and temperature at constant levels during storage. Paper should demonstrate a relative humidity from 50 % to 55 %; the temperature should be constant between 20 °C and 22 °C (68 °F and 71.6 °F). Crease Formation
  • 6. 6 Should creases develop, this may also be the fault of incorrect machine settings – most likely on the sheet-feeder. Among the reasons creases may form are incorrectly set or jamming front lays, side lays that draw with too much force, a hold-down device that has been set too tightly, or an air-blast that is too strong. An incorrect air-pressure setting at the point of sheet transfer may also contribute to the formation of creases. Further sources include poorly functioning or dirty grippers, which warp the sheet, as well as a printing pressure between the rubber and the impression cylinder that is set too high, or is uneven. This tumbles the sheet, and will result in creasing. …Continued
  • 7. Remedy •Employ printing stock that is good and flat • Inspect the front lays • Inspect the side lays • Do not set the hold-down device too tightly • Reduce the air-blast on the sheet-feeder • Optimize the air-pressure adjustments at the point of sheet transfer • Optimize the print lateral feed • Inspect, clean, and adjust the grippers as needed
  • 8. Picking occurs when small particles are torn out of the surface of the paper, or printing stock rips during the printing process. This can cause damage to the printing blanket. It becomes necessary to wash more frequently, and print quality is adversely affected. Picking becomes a problem when surfaces are not sufficiently resilient. This indicates that the tractive force of the printing ink is greater than the fiber adhesion in the paper structure, or the bonding of the pigment used in the coating. Inadequate gluing, or the poor anchoring of the coating material on the paper’s surface may cause picking Picking
  • 9. Remedy • Employ a soft series of inks • Reduce the ink’s tractive force (add printing oil) • Allow the machine to run on standard working condition • Raise the rasp temperature (temper the inking system) • Reduce the speed of the machine; this lessens the traction on the paper • Use a quick release blanket • Employ paper of better quality
  • 10. Emulsification Emulsion is a mixture of ink and dampening solution. In this process, Dampening solution is distributed evenly throughout the ink in small droplets. The proportion of water in a “stabile emulsion” is around 20 %. If higher, then the ink’s splitting properties are reduced, and the ink flow is interrupted. As a result, the emulsion becomes unstable, the ink “builds up”, and it “emulsifies”. Too large a proportion of dampening solution in the printing ink, or too low a pH-value fosters emulsification. Printing inks react differently, depending on what type they are: blended inks, dayglo, or metallic inks are more sensitive than inks in the normal scale. Emulsified printing inks will increase drying times, as well as increasing the risk of deposits.
  • 11. Remedy • Set the ink and dampening balance correctly, and check on it continuously throughout the printing process. • In case of emulsified ink, wash the rollers, and re-establish the smearing limit. • Check the dampening solution, and change it regularly (the ideal dampening solution has a water hardness from 8 to 12° dH, a pH-value from 4.8 to 5.5, and a temperature from 10 °C to 15 °C (50 °F to 59 °F). • On an Alcolor dampening unit: separate the intermediate roller from the inking unit; install cross-flow ventilators. • Avoid frequent phases of pre- and post-dampening (during make-ready or stoppages). • Inspect and optimize the adjustment of the inking and dampening rollers. • Where there is less ink taking, an additional ink stripe may be introduced to stabilize the balance of ink and water
  • 12. Ghosting By ghosting, one understands a circumstance where printing form elements other than the desired positive or negative ones duplicate themselves onto the printed surface. These “stencils” or “ghost images” emerge from repeated passes of the ink form roller over the plate cylinder, and from a reduction or accumulation of ink. Used (hard) or poorly adjusted ink-rollers facilitate ghosting, and the tendency toward ghosting increases with weak pigment inks. An optimal balance between ink and dampening solution helps prevent ghosting, since too much water negatively influences printing outcomes.
  • 13. Remedy • When maintaining rollers, only use the appropriate cleansing agents; a weekly application of wash paste removes lime deposits, and will regenerate the rollers. • Adjust the rollers in accordance with the instruction manual; inspect the adjustment regularly. • Change used rollers: the rubber surface of older rollers will become glossy and over-smooth. At the same time, as their hardness increases, the edges bulge out in a trumpet shape. More pronounced abrasion becomes evident. • Adjust for maximum lateral distribution.
  • 14. …Continued • Adjust reciprocation of the ink form rollers • Shift the engaging point of the lateral distribution • Reduce the quantity of dampening solution being used (smearing limit) • Employ high pigment inks • Turn on the vario • Turn the printing form (prepress)
  • 15. Mottling When speaking of “mottling” or “back trap mottling“, printers are referring to a cloudy print output. The problem originates in paper that is partially uneven, and the resulting uneven absorption and back split characteristics. If the paper is spotted, or if a certain amount of cloudiness is already present in the coating, then the printing ink will be only partly absorbed. In 4-color Sheetfed offset printing, the printing result will back split on the printing blankets of the subsequent printing units. When an uneven penetration of printing ink is especially pronounced, this will become visible after the back split process occurs, as an uneven print reproduction. The problem of a “cloudy printout” manifests itself in the greatest variety in offset printing. In order to isolate the printing paper as the culprit, one must first determine if the visual appearance of the cloudy printout matches up with the paper structure. This can be done using backlighting, or under UV light. The absorption characteristics of the printing ink on the paper in question can also be made visible by resorting to a simple wipe test using special wipe-test ink. In this way, the proof that paper is the root cause may be adduced.
  • 16. Remedy In cases where the cloudy printout is purely the result of the paper being used, the only solution is to change to an alternative type of paper.
  • 17. Horizontal Stripes The problem in this case involves disturbances in the printed image, which are manifested as bright or dark stripes running horizontally to the direction of printing. Horizontal stripes arise for a variety of reasons. Besides adjustment errors, errors in screen vignettes (prepress errors) may also play a role. Additionally, the formation of stripes may also be influenced by contamination from the build up of powder and coating, from damage to the printing blanket or the printing plate, or from the ink/dampening solution feeds, as well as from the quality of the ink. The machines themselves may also be causing the stripes, for example from an incorrect alignment of the ink and dampening units, or from rolling errors (too much pressure). Tone stripes can be caused by the relative lateral movement of the rollers on the printing plate.
  • 18. Remedy for stripe formation conditioned by machines • When maintaining the rollers, only use appropriate cleansing agents; the weekly application of a wash paste removes lime deposits, and will regenerate the rollers. • Adjust the rollers in accordance with the instruction manual; inspect the adjustment regularly. • Change used rollers: the rubber surface of older rollers becomes glossy and over-smooth. At the same time, as their hardness increases, the edges bulge out in the shape of a trumpet. More pronounced abrasion becomes evident. • Adjust reciprocation of the ink form rollers • The dampening distributing cylinder must be kept clean and receptive to water. • The roll bearings must be in fine working condition (no play, no sticking). • Lubricate the roll bearings.
  • 19. …Continued • By setting the ink form rollers as gently as possible on the printing plate, impacts stemming from the run-on and run-off edges are reduced. • The bearer ring should be kept clean and grease-free. • The calibrated underpacking should be clean, cut in a format to fit, and correctly inserted. • Clamping between the plate and the blanket should range between 0.1 mm and a max. 0.13 mm. (0.004 in and 0.051 in). • Clamping between the blanket and the counterpressure should be set in consideration of the surface of the printing stock; avoid clamping that is set too high.
  • 20. Darkening When darkening occurs, the darker colors are transferred from the blanket over the printing plate onto the succeeding inking system, where they contaminate the light colors. During wet-on-wet printing, the tackiness of the inks must be coordinated. Nevertheless, it can happen that the darker colors from the first printing units contaminate the lighter colors (mainly yellows) in the latter printing units.
  • 21. original tone color after blanket contamination Remedy • Change to a different kind of ink • Deposit the lighter colors more in the direction of the sheet-feeder. • Follow the rule of thumb “screen before surface” for the inking sequence. • Raise the dampening solution feed in the lighter colors, or increase the lighter colors.
  • 22. Decrease in Tone Value The reduction of the halftone dot in the print when compared to the original (film, printing plate) is referred to as a decrease in tone value. This phenomenon may already arise in prepress. In addition, various parameters can also have a bearing on abrasion of the printing plate: • Normal plate wear and tear • Coating build up or powder deposits on the blanket • Unsuitable plate cleanser (admixture of abrasive material)
  • 23. …Continued • A pH-value in the dampening solution that is too low may slightly etch the edges of the halftone dots. • An alcohol content that is too high corrodes the ink-accepting coating. • Rapidly volatizing cleansing solutions may damage the printing plate.
  • 24. Remedy • Employ appropriate printing plates • Use a suitable plate cleanser and certified cleaning solution when Maintaining the printing plate. • Avoid using abrasive powder (calcium carbonate) • Always prepare dampening solution according to instructions (pH-value, alcohol concentration); the ideal dampening solution has a water hardness of 8 to 12° dH, a pH-value of 4.8 to 5.5, and a temperature Ranging from 10 °C to 15 °C (50 °F to 59 °F).
  • 25. Increase in Tone Value An increase in tone values means a gain in the halftone dot of the print compared to the original (film, printing plate). In order to establish an increase in tone value, a full tone field combined with a defined grid is needed. The problem of an increase in tone value may already arise during the preparation of the printing form. While an increase in tone value in a printing press cannot be entirely avoided, it should never be allowed to exceed a certain point. An increase in tone value depends on type of ink, ink quantity, the temperature in the inking system, the surface of the printing stock, the clamping, the blanket type, the dampening solution, and the quantity of dampening solution employed.
  • 26. Remedy • Print with a familiar ink series, if possible without additives, within the tolerance levels of your own standards of density. • An increase in tone value (approx. 2 %) must be taken into consideration during black and white printing. • Employ appropriate black and white inks • Set the inking system between 27 °C and 30 °C (80 °F and 86 °F) • Avoid changing the printing stock during the print run
  • 27. …Continued • Clamping between the plate and the blanket should be set between 0.1 mm and max. 0.13 mm (0.004 in and 0.051 in) • Pressing between the blanket and the counterpressure should be set to reflect the printing stock surface; avoid setting compression too high. • A fixed type of blanket should be used in the pressroom (standardization) • Only use certified cleansing solutions when washing. • Wash new blankets with water after mounting in order to remove the talcum. • Newly stretched blankets must be restretched. • Run the quantity of dampening solution slightly over the smear limit, and precisely maintain the balance of ink and dampening solution. • Optically test the three-quarter tones with a line tester.
  • 28. % TWZ for CMY including tolerances TWZ for K including tolerances 40 13,0 +/– 3 16,0 +/– 3 50 14,3 +/– 3 17,0 +/– 3 70 13,4 +/– 3 14,9 +/– 3 80 10,7 +/– 3 11,5 +/– 3 ISO Standard Values
  • 29. Slurring One speaks of slurring when the geometry of the halftone dot changes. The printed image then appears to be displaced. The round halftone dot assumes an oval shape. Two types of slurring exist – on the one hand, in the direction of printing (circumferential slurring), and on the other hand, transverse to the direction of printing (lateral slurring). These effects lead to a reduction in quality, and reflect the processing conditions within the group comprising the plate, blanket, and printing cylinders, as well as on other material influences.
  • 30. Remedy • Check the printing pressure adjustment, and reduce as needed • Maintain recommended packing thicknesses (control with a cylinder gauge) • Mount the blankets carefully, and use a torque wrench when stretching • Insert the blankets in the printing press in the indicated weave direction • Clean the grippers and adjust them as needed
  • 31. Lags in Drying If the ink dries too slowly in the stack, one speaks of a lag in drying time. This may lead to an ink rub-off of the print during print finishing or during transport. The interaction between ink, additives, and dampening solution is usually to blame for lags in drying time. For example, should the pH-value of the dampening solution fall below 4.7, one can count on a longer drying time. Incorrectly dosed additives (drying accelerators), a stack temperature that is too low, or excessively emulsified ink also retards drying. In principle, the heavier the ink film, the slower the drying process.
  • 32. Remedy • Optimal tuning between ink and paper (inquire with the manufacturer) • Do not allow the pH-value of the dampening solution to cross below 4.7 • Avoid ink emulsification • Only dose additives according to the manufacturer’s indications • In cases of lower ink taking, also print ink stripes • Avoid high ink film densities (employ ink reduction or high pigment inks) • Use IR drying • In order to rescue a print job, coat it with an oil or dispersion varnish
  • 33. 33 Contact Us Mr. Rajendra Prasad. Rajendra.prasad@heidelberg.com www.heidelberg.com Copyright © 2014 Heidelberg India, All rights reserved. Heidelberg India Keeps members of Printing industry informed About its latest development and attractive offers.